La hoja de flujo de extracción de cromita

Chromite Ore Crushing
The crushing section for this 250 ton per day chrome mill consists of a coarse ore grizzly, a coarse ore bin with pan feeder to a 1’8″ reduction crusher and a crusher discharge conveyor to a crushed ore bin. On this particular ore, we find that there is no chrome liberated in sizes larger than ¼”.

Accordingly the crusher discharge opening is ¾” and the minus ¼” material is removed for concentration before further reduction.

Chromite Grinding
The 36″x 8′ Adjustable Stroke Ore Feeder is used to accurately control feed of crushed ore to the grinding section. Before it is fed to the 4’x 8′ Peripheral Discharge Rod Mill, the minus ¼” chrome ore is removed from the grinding circuit by means of a 4’x 12′ Dillon Vibrating Screen. This minus ¼” product is then ready for concentration in the Mineral Jigs.

La criba vibratoria de gran tamaño se muele en el molino de varillas con cabezal de acero. Se prefiere un molino de barras con la función de descarga periférica para esta aplicación porque el diseño de «paso rápido» produce un mínimo de finos indeseables. La descarga del molino de varillas vuelve a la criba vibratoria Dillon por medio de un elevador de cangilones de correa, de modo que se obtiene una disposición de rectificado de circuito cerrado.

Dillon
Gravity Recovery Section
The minus ¼” undersize from the Vibrating Screen is divided to feed two identical, parallel jigging circuits, each consisting of l6″x 24″ Duplex Mineral Jig used for roughing and a I6″x 24″ Duplex Mineral Jig used as a scavenger. Automatic Density Discharge Control Valves on the hutches of the scavenger Mineral Jig provide a controlled, continuous, high-density feed to a l6″x 24″ Duplex Mineral Jig used for final cleaning.

A final, cleaned concentrate is produced by the two cleaner Mineral Jigs and also a middling product which is re-circulated back to the scavenger jigs. This procedure is preferable to the immediate regrinding of the middlings as it avoids the further reduction of relatively pure chrome particles which are bound to be present.

The tailing from the scavenger Mineral Jig is directed to a 30″x 13′ Simplex Cross-Flow Classifier which discards a waste product as a final tailing at minus 65 mesh and the sand product is returned to the rod mill for further grinding. A SRL Sand Pump is used to pump the Mineral Jig Tailings to the Cross-Flow Classifier.

Chromite Process Summary
This flowsheet is very effective due to the ability to remove the high grade chrome with very little grinding on each pass through the mill. In this way, grinding takes place with a large number of small reductions followed by immediate removal of the liberated chrome into a high grade concentrate.

In the concentration of certain chrome ores, high grade chrome particles are sometimes liberated at sizes larger than ¼”, For the concentration of these large size chrome particles, the Improved Harz Type Jig is indicated.

In the flowsheet described here, there is a minimum amount of valuable chrome in the classifier overflow and accordingly this product is sent to waste. However, conditions may justify the installation of slime concentrating tables and Tilting Concentrators.